RE: Questions on DuraForm GF and other options

From: Tony Furdock (tonyf@3dresource.com)
Date: Thu Mar 07 2002 - 18:05:38 EET


Questions on DuraForm GF and other options
Mike -(and everyone else who's interested) -

We often build water-tight parts with Duraform GF infiltrated with Imprex
Superseal(TM). This stuff is water-thin, and we immerse the part(s) in a tub
of the superseal in a vacuum chamber. We take them out when the bubbles stop
coming out of the part, and cure them in an oven at 150F for about an hour
(depending on part size and thickness). This process has yielded parts up to
an inch thick being completely infiltrated.

Good luck, and let me know if you have any other questions.

Tony
Tony Furdock
Creative Technical Solutions
6880 Hillsdale Court
Indianapolis, IN 46250
317-578-3445
fax 317-578-3446
www.3dresource.com

_________________________________________________

This e-mail and any attached file is intended only for the person or entity
to which it is addressed and may contain information that is privileged,
confidential or otherwise protected from disclosure. Dissemination,
distribution or copying of this e-mail or the information herein by anyone
other than the intended recipient, or an employee or agent responsible for
delivering the message to the intended recipient, is prohibited. If you have
received this email in error, please immediately notify us by calling the
person listed above.

_________________________________________________

  -----Original Message-----
  From: owner-rp-ml@rapid.lpt.fi [mailto:owner-rp-ml@rapid.lpt.fi]On Behalf
Of Pacholski, Mike [SAA]
  Sent: Wednesday, March 06, 2002 5:51 PM
  To: 'rp-ml@rapid.lpt.fi'
  Subject: Questions on DuraForm GF and other options

  List,
          I was wondering if someone could help me with my question. I'm
looking at making a testable prototype from an SLS with DuraForm GF. The
questions is regarding the finishing process. One options is a vacuum
impregnating the part with a Methacrylate resin the other is treatment of
Cyanocrylate. What is the difference and effect of these two process? I will
be running the part in water and machining it down in between my tests.

          Also, are there any better materials (e.g.. strong and more
durable) than the DuraForm GF that can be tested in water that I should be
looking into? (not including steel RP, the build area is not large enough)
The Stratasys Polycarbonate and Polyphenylsulfone also looked like an
option, but I still need to do more research on this.

  Your comments and suggestions will be greatly appreciated.

  Thanks in advance,

  Mike